COMPOSITION AQUAMET® 17 AQUAMET ®19 AQUAMET® 22
Carbon 0.07 max 0.80 max 0.06 max
Manganese 1.00 max 2.00 max 4.00 - 6.00
Silicon 1.00 max 1.00 max 1.00 max
Chromium 14.50 - 16.50 18.00 - 20.00 20.50 - 23.50
Nickel 3.00 - 5.00 8.00 - 10.50 11.50 - 13.50
Phosphorus 0.04 max 0.04 max 0.04 max
Sulfur 0.03 max 0.03 max 0.03 max
Copper 3.00 - 5.00
Columbium + Tantalum 0.15 - 0.45 0.10 - 0.30
Nitrogen 0.20 - 0.30 0.20 - 0.40
Molybdenum 1.50 - 3.00
Vanadium 0.10 - 0.30
Iron Balance Balance Balance

Mechanical Properties
Tensile Strength Psi 0.2 % Yiield Tension psi Strenth Torsion psi Elongation in 2 in . % Reduction of Area %
AQUAMET® 17
Up to 8 " 135,000 105,000 70,000 16 50
8" to 12 " 135,000 105,000 70,000 12 35
AQUAMET® 19
Up to 1½" 130,000 105,000 70,000 20 55
Over 1½" to 2" 115,000 85,000 57,000 25 55
55Over 2" to 2½" 105,000 60,000 40,000 30 55
Over 2½" to 3" 100,000 55,000 36,000 35 55
Over 3" to 12" 95,000 50,000 33,000 35 55
AQUAMET® 22
¾" to 1¼ " 145,000 130,000 86,600 18 45
Over 1¼" to 2" 135,000 105,000 70,000 20 50
Over 2" to 2½ " 120,000 95,000 63,000 20 50
Over 2½" to 3" 115,000 75,000 50,000 25 50
Over 3" to 12" 100,000 55,000 36,600 30 50
AQUAMET® 22 H.S.
2½ " to 6" 130,000 105,000 70,000 15 45
Minimum values. Actual test results may be higher.